Unknown - page 902

D310
Multi Function
ISO
Material
Condition
Tensile
Strength
(N/mm2)
Hardness
HB
Cutting speed: Vc (m/min)
min
max
Non-alloy steel
and cast steel,
free cutting steel
< 0.25 %C
Annealed
420
125
260
280
≥
0.25 %C
Annealed
650
190
200
230
< 0.55 %C Quenched and tempered
850
250
160
190
≥
0.55 %C
Annealed
750
220
160
180
≥
0.55 %C Quenched and tempered
1000
300
140
160
Low alloy steel
and cast steel
(less than 5% all elements)
Annealed
600
200
160
190
Quenched and tempered
930
275
120
140
Quenched and tempered
1000
300
130
150
Quenched and tempered
1200
350
140
160
High alloy steel,
cast steel, and tool steel
Annealed
680
200
130
160
Quenched and tempered
1100
325
70
90
Stainless steel and cast steel
Ferritic / martensitic
680
200
110
200
Martensitic
820
240
60
180
Austenitic
600
180
80
120
Cast iron nodular (GGG)
Ferritic / pearlitic
-
180
80
260
Pearlitic
-
260
130
240
Grey cast iron (GG)
Ferritic
-
160
150
280
Pearlitic
-
250
90
280
Malleable cast iron
Ferritic
-
130
150
280
Pearlitic
-
230
140
240
Aluminium-wrought alloy
Not cureable
-
60
810
840
Cured
-
100
730
830
Aluminium-cast, alloyed
≤
12% Si
Not cureable
-
75
800
840
Cured
-
90
730
830
> 12% Si
High temperature
-
130
320
340
Copper alloys
> 1% Pb
Free cutting
-
110
400
430
Brass
-
90
400
430
Electrolitic copper
-
100
270
300
Non-metallic
Duroplastics, fiber plastics
-
-
-
-
Hard rubber
-
-
-
-
High temp. alloys
Fe based
Annealed
-
200
20
40
Fe based
Cured
-
280
20
30
Ni or Co based
Annealed
-
250
20
30
Ni or Co based
Cured
-
350
20
30
Ni or Co based
Cast
-
320
30
70
Titanium and Ti alloys
RM 400
-
30
70
Alpha + beta alloys cured RM 1050
-
30
70
Hardened steel
Hardened
-
55 HRC
30
50
Hardened
-
60 HRC
30
40
Chilled cast iron
Cast
-
400
60
80
Cast iron
Hardened
-
55 HRC
30
50
MACHINING DATA FOR SHREDMEISTER ROUGHER ENDMILLS